How to Drill Hardened Steel: HSS, Cobalt or Carbide?

The short answer:

Tough steel: M42 cobalt. Properly hardened steel: a TCT carbide drill bit, slowly, in a rigid setup.

HSS will skate on hardened steel and cobalt struggles once the steel is above about 45 HRC. A tungsten carbide tipped bit will cut it, but carbide is brittle, so the setup has to be rigid and the speed low. Cutting fluid, firm steady pressure, and never freehand on a loose workpiece.

“Nothing will drill this” usually means one of two things: the steel is hard but not hardened (stainless, high-alloy, high-tensile) and the wrong bit was used, or the steel is properly hardened (a security plate, a hardened pin, a file, a bearing race) and only carbide will touch it. Telling the two apart saves a lot of bits.

Is my steel hard, or hardened?

Run a file across it. If the file bites, it is tough steel and cobalt will drill it. If the file skates, it is hardened and you need carbide.

The file test is the one we give over the phone. A good file is around 60 HRC. If it cuts a mark, the steel is below that and an M42 cobalt bit (hardness around 67 HRC) will drill it with care. If the file slides off and polishes the surface, the steel is in the same range as the file, and only tungsten carbide (over 80 HRC) will cut it.

Typical “hard but not hardened”: stainless, high-tensile bolts (8.8 and 10.9), chrome-moly, tool steel in its annealed state. Typical “hardened”: 12.9 bolts, security plates, hardened pins and dowels, files, springs, bearing races, hard-faced wear plates.

What drill bit do I need for hardened steel?

A TCT (tungsten carbide tipped) drill bit. Carbide is the only common bit material harder than hardened steel.

A TCT drill bit has a tungsten carbide tip brazed onto a steel body, in the same way an SDS bit does, but ground to cut metal. It drills hardened steel, hard-faced plate, cast iron skin and other materials that destroy HSS and cobalt. It does not replace cobalt for everyday metalwork: carbide is brittle, so on soft or flexing material it chips where a cobalt bit would simply cut.

Material Bit Notes
Mild steel, aluminium HSS Standard speed and fluid
Stainless, 8.8 bolts M35 cobalt Half speed, firm pressure, fluid
Tough alloy, 10.9 bolts, thick stainless M42 cobalt Slow, rigid, fluid
Hardened steel, 12.9 bolts, security plate, springs TCT carbide Very slow, rigid, no flex, fluid

How do I drill hardened steel without chipping the bit?

Slow speed, a rigid setup, firm and constant pressure, cutting fluid, and no sideways load at all.

1
Clamp everything. Carbide snaps under sideways load. The workpiece must not move and the drill must not wander. A pillar drill or mag drill is ideal; a hand drill will do if the work is clamped and you can hold the drill square and steady.
2
Go slow. Roughly a third of mild-steel speed. For a 6mm TCT bit that is around 400–500 RPM; for 10mm, 250–300. See our drill speed chart.
3
Keep it cutting. Firm, even pressure so the tip is always taking a chip. Let it rub and the steel work-hardens further under the tip. Do not peck in and out.
4
Use cutting fluid. Carbide tolerates heat better than HSS, but the braze and the workpiece do not. Fluid keeps the edge cool and stops the surface glazing.
5
No pilot hole. Unlike HSS, a carbide tip prefers to start on solid material. A pilot hole leaves the fragile tip corners to do the work and they chip. Start the full-size bit on a centre-punch mark.
6
Ease off at breakthrough. The point breaking through the back face is when carbide chips most. Back the pressure right off for the last millimetre.

Can I drill a hardened bolt or pin out?

Yes, with a TCT bit, centre-punched and clamped, slowly. Or anneal it first with heat if the surrounding material allows.

A sheared 12.9 bolt or a hardened dowel is the classic job. Grind the stub flat, centre-punch it dead centre, and drill with a TCT bit a size or two under the thread minor diameter, slowly with fluid. Once through, the remains usually pick out or come with an extractor.

If you can get heat on it without damaging what is around it, heating the stub to cherry red and letting it cool slowly (annealing) softens it enough for a cobalt bit. On an alloy casting or near a seal, do not.

Will a cobalt bit drill hardened steel?

Not reliably. M42 cobalt sits around 67 HRC and will cut tough steel up to roughly 45 HRC. Above that it rubs, overheats and blunts.

Cobalt is the right bit for most jobs people call “hard”: stainless, high-tensile bolts, alloy steel, cast iron. It is the wrong bit once the steel is actually hardened. If you have already tried a sharp M42 bit, slowly, with fluid, and it polished the surface without cutting, that is your answer: go to carbide. Our M35 vs M42 guide covers where cobalt stops.

How we know: we have supplied drill bits to UK trade and industry since 1985. In the last 12 months we sold around 15,000 packs of M35 cobalt and 6,750 TCT drill bits. The TCT bits go mostly to engineers, locksmiths and fabricators dealing with hardened material; the “won’t drill” calls nearly always resolve with the file test above.

Cobalt and TCT drill bits, from stock

M35 and M42 cobalt in every size, plus TCT carbide drills for hardened steel. Same-day dispatch from Wigan, free next-working-day UK delivery on orders over £50.

TCT drill bits · M42 cobalt · M35 cobalt · Drilling stainless

Frequently asked questions

What is the best drill bit for hardened steel?

A TCT (tungsten carbide tipped) drill bit. It is the only common bit material harder than hardened steel. Use it slowly, clamped rigid, with cutting fluid and no sideways load.

Can a cobalt drill bit drill hardened steel?

Only if the steel is tough rather than truly hardened. M42 cobalt handles up to roughly 45 HRC (stainless, 10.9 bolts, alloy steel). Above that it rubs and blunts; use carbide.

How do I tell if steel is hardened?

Run a file across it. If the file bites, cobalt will drill it. If the file skates and polishes the surface, the steel is hardened and you need a TCT carbide bit.

What speed do I drill hardened steel at?

About a third of mild-steel speed: around 400–500 RPM for a 6mm bit, 250–300 for 10mm. Firm constant pressure and cutting fluid, and back off at breakthrough.

Should I drill a pilot hole in hardened steel?

No. A carbide tip starts best on solid material from a centre-punch mark. A pilot hole leaves the fragile tip corners doing the work and they chip.

Can I drill out a hardened bolt?

Yes. Grind the stub flat, centre-punch it, clamp the work and drill with a TCT bit a size under the thread minor diameter, slowly with fluid. Heating to cherry red and cooling slowly first softens it enough for cobalt if the surroundings allow.

UK Drills has supplied drill bits to UK trade and industry since 1985, from our trade counter in Hindley, Wigan. Not sure what you need? Email info@ukdrills.com — we’re happy to advise.